Tin Bronzes – CuSn10
EN 1982 CC480K
CuSn10-C
It is a tin bronze alloy.
International standards ASTM B505 C90700 and C92700
Chemical Composition
Cu % | Ni % | P % | Pb % | Sn % | Zn % | A1 % | Fe % | Mn % | S % | Sb % | Si % |
---|---|---|---|---|---|---|---|---|---|---|---|
Min. 88 Max. 90 | Max. 2 | Max. 0,2 | Max. 1 | Min. 9 Max. 11 | Max. 0,5 | Max. 0,01 | Max. 0,2 | Max. 0,01 | Max. 0,05 | Max. 0,02 | Max. 0,02 |
Mechanical Properties
Hardness HB | Yield Strength (MPa) | Tensile Strength (MPa) | Elongation % | Hardness (HBW) |
---|---|---|---|---|
Continuous Casting | 280 | 170 | 10 | 80 |
Centrifugal Casting | 280 | 160 | 10 | 80 |
Physical Properties
Density (kg/dm3) | Specific Heat Capacity (J/(gr.K)) | Thermal Expansion (10-6k) | Thermal Conductivity (W/(m.K)) | Electrical Conductivity (Ω mm²/m) |
---|---|---|---|---|
8,7 | 0,376 | 18,5 | 59 | 7 |